Laboratory accredited by GAZ, (Association for the Accreditation and Certification GmbH) Attestation no. 91021

CERTIFIED REFERENCE MATERIAL
SX32-34
BF-slag

Version: 004      Date of certification: 08.10.12      Sample form: Powder < 0.125 mm

Analyte Unit Certified value Confidence
interval (95%)
No. of independent
repeated series
Measuring
method*
  CaO
SiO2
Fe
Mn
S
  %
%
%
%
%
     37.22
41.28
0.742
0.970
0.88
      0.10
0.23
0.004
0.003
0.02
 4
4
6
6
8
1
1
1
1
1,2
  Al2O3
MgO
TiO2
Na2O
K2O
  %
%
%
%
%
     11.27
5.37
0.618
0.322
0.890
      0.05
0.02
0.004
0.001
0.003
 5
6
5
3
5
1
1
1
3
1
  SrO
BaO
ZrO2
V2O5
Cr2O3
  %
%
%
%
%
      0.048
0.087
0.042
0.016
0.018
    < 0.001
0.002
0.003
0.001
0.003
 5
5
3
3
3
1
1
1
1
1
* Measuring method
1: X-ray fluorescence spectrometry
2: Combustion with IR-detection
3: Atomic absorption spectrometry
 

Comment
Thermal treatment of material before weighing: 105°C, 1 h