Laboratorium
Postfach 1580, 66748 Dillingen
CERTIFIED REFERENCE MATERIAL
SX02-11
Cement

Version: 003      Date of certification: 04.09.25      Sample form: Powder < 0.100 mm
Analyte Unit Certified value Confidence
interval (95%)
No. of independent
repeated series
Measuring
method*
  Ca
SiO2
Fe2O3
Mn3O4
P2O5
  %
%
%
%
%
     40.63
25.04
2.98
0.172
0.137
      0.06
0.16
0.01
0.002
0.002
 6
4
5
6
4
1
1
1
1
1
  S
Al2O3
MgO
TiO2
Na2O
  %
%
%
%
%
      1.48
6.86
2.79
0.319
0.156
      0.04
0.03
0.01
0.004
0.004
 5
6
6
6
3
1
1
1
1
2
  K2O
Be
SrO
BaO
La
  %
%
%
%
%
      0.524
0.00031
0.083
0.041
0.0047
      0.002
0.00001
0.001
0.002
0.0001
 4
4
3
4
4
1
3
1
1
3
  Zr
V
Cr
Mo
Co
  %
%
%
%
%
      0.0133
0.0077
0.0032
0.00020
0.00076
      0.0023
0.0002
0.0002
0.00002
0.00004
 4
7
3
4
4
3
1,3
3
3
3
  Ni
Cu
Zn
Cd
In
  %
%
%
%
%
      0.00207
0.0065
0.0402
< 0.00004
< 0.00004
      0.00005
0.0003
0.0014
-.-
-.-
 4
4
7
4
4
3
3
1,3
3
3
  Tl
Pb
As
Sb
Bi
  %
%
%
%
%
    < 0.00006
0.00293
0.00269
0.00016
< 0.00003
      -.-
0.00013
0.00027
0.00002
-.-
 4
4
4
4
4
3
3
3
3
3
  Se
Te
Ce
Th
U
  %
%
%
%
%
      0.00016
< 0.00014
0.0065
0.00083
0.00057
      0.00004
-.-
0.0003
0.00002
0.00001
 3
4
4
4
4
3
3
3
3
3
* Measuring method
1: X-ray fluorescence spectrometry
2: Atomic absorption spectrometry
3: ICP with high resolution mass spectrometry
 

Comment
Thermal treatment of material before weighing: 800°C, 1 h