"Excellence Laboratory Technische Compliance Level III" by GAZ GmbH (Attestation no. GAZ-TCL-12-02-14-01)

CERTIFIED REFERENCE MATERIAL
SL23-12
Fe-Si

Version: 004      Date of certification: 04.01.17      Sample form: Powder <0.200 mm
Analyte Unit Certified value Confidence
interval (95%)
No. of independent
repeated series
Measuring
method*
  Ca
Si
Fe
Mn
P
  %
%
%
%
%
     10.48
48.30
12.38
0.114
0.011
      0.05
0.05
0.09
0.003
< 0.001
 3
3
3
2
5
1
1
1
1
1,2
  S
Al
Mg
Ti
Cr
  %
%
%
%
%
      0.056
3.40
0.193
0.062
0.076
      0.001
0.02
0.010
0.004
0.008
 3
3
3
3
4
1
1
1
1
1,2
  Ni
Cu
C
  %
%
%
      0.013
0.020
4.96
      0.001
0.001
0.02
 5
5
3
1,2
1,2
3
* Measuring method
1: X-ray fluorescence spectrometry
2: ICP with high resolution mass spectrometry
3: Combustion with coulometric detection